Application
News
No. V28
High-Speed Video Camera Hyper Vision HPV-X2
3D-DIC Analysis in Impact Test of Silicon Wafer
LAAN-A-HV-E013
As the main material for semiconductor devices, silicon wafers
(hereinafter, Si wafers) are the most important basic material in
the electronic industry. Si wafers are manufactured by applying
polishing, heat treatment and other processes to thin sheets
(wafers) sliced from single crystal ingots of silicon (Si).
In recent years, demand for semiconductor devices such as
flash memories and LSIs has increased explosively, and higher
throughput is also required in the manufacturing process in
order to satisfy this continually-increasing demand. Use of
larger-diameter Si wafers is progressing with the aim of
increasing the number of devices that can be manufactured
from each Si wafer, and this has made large contributions to
both higher throughput and cost reduction.
However, recent Si wafers have reached a size of φ300 mm but
have a thickness of only 1 mm or less, and great care is
necessary in handling these hard, brittle Si wafers.
An accurate knowledge of the size and distribution of strain at
the wafer surface until a Si wafer is destroyed is necessary in
order to improve wafer handling technologies, but because
destruction of Si wafers is a high-speed phenomenon,
adequate information could not be obtained with the
conventional techniques.
In this example, high-speed deformation of Si wafers was
visualized by 3D-DIC analysis*
1
by observing the destruction of
Si wafers from two directions using two Hyper Vision HPV-X2
high-speed video cameras.
F. Yano
*1 DIC (Digital Image Correlation) analysis:
Technique for investigating the amount of pattern movement
at the surface of an object by comparing a random pattern
before/after deformation. Three-dimensional measurement
(3D-DIC) from images taken from two directions is also possible.
Measurement System
In a puncture test using a High-Speed Puncture Impact
Testing Machine HITS-P10, destruction was observed with
two Shimadzu Hyper Vision HPV-X2 high-speed video
cameras. Because the two HPV-X2 cameras are connected
with a synchronization cable, synchronized recording in
which the phases of the recording frames coincide is possible.
Recording from two directions enables highly accurate 3-
dimensional measurement considering deformation in the
out-of-plane direction.
The test equipment used in this example is shown in Table 1.
Fig. 1 shows the arrangement of the test equipment, and
Fig. 2 shows the condition of the test section. To observe the
opposite side to punching side of the specimen by striker
from the front of the device, a plane mirror is arranged at the
bottom of the test section. Recording is triggered by
detection of the position where the striker contacts the
specimen so as to match the timing of recording.
As the images taken by the HPV-X2 cameras are analyzed by
using the DIC software VIC-3D, it is possible to obtain the
distribution of displacement. With VIC-3D, the HPV-X2 cameras
are controlled directly by the DIC software, and as a result, the
complicated calibration operation which is essential in 3D-DIC
and data analysis at the time of measurement can be
performed easily.
Table 1 Measurement Conditions
High-speed video camera :Hyper Vision HPV-X2 × 2 units
Testing system : High-Speed Puncture Impact Testing
Machine HITS-P10
Lighting : Strobe
DIC software : VIC-3D (Correlated Solutions, Inc.)
Fig. 1 Arrangement of Test Equipment
Fig. 2 Condition of Test Section
Test Conditions
A 3-inch Si wafer with a <100> crystal orientation was used as
the test specimen. Table 2 shows the details of the specimen. A
random pattern was drawn on the satin-finished surface of the
Si wafer with a permanent (oil-base) marker (Fig. 3). The test
conditions are shown in Table 3.
Test section
HPV-X2 (R)
HPV-X2 (L)
Striker
Specimen
Mirror