Application
News
No. i270
Precision Universal Testing Machine
Tensile Test of High Tensile Strength Steel
LAAN-A-AG-E029
High tensile strength steel is a class of materials with
increased strength in comparison with general structural
steels, and materials with strengths of 1,000 MPa or more
have also been developed. High tensile strength steel is
mainly used in the automotive industry, where it has
attracted attention due to heightened awareness of
environmental problems and demands for collision
safety. In particular, auto body weight reduction for
improvement of fuel economy is one effective
countermeasure for the global warming of recent years,
and this increased the momentum toward adoption of
high tensile strength steel, which makes it possible to
obtain the same strength as general steel materials with
thinner gauge products.
The evaluation items for metallic materials include
tensile strength and elastic modulus. These mechanical
properties are measured in accordance with the material
testing standards ISO 6892-1 and JIS Z 2241. As described
in this article, a tensile test of high tensile strength steel
using strain rate control was conducted in accordance
with JIS Z 2241 Annex JB. In addition, hydraulic flat grips
with high gripping force were used to enable testing of
the high tensile strength steel without slipping in the
grips.
F. Yano
Measurement System
In this test, a Shimadzu AGX™-V Series precision universal
testing machine was used. Because the elastic modulus
was also measured in this test, we used a Shimadzu SSG-
H Series strain gauge extensometer, which enables
highly accurate measurement of the elongation in the
gauge length of the specimen. The specification of the
test system used here is shown in Table 1, and the
condition of this test is shown in Fig. 1.
Table 1 Specification of Test System
Instrument : AGX-100 kNV
Grip : Hydraulic flat grip
Extensometer : SSG50-10H
Software : TRAPEZIUM X-V
Fig. 1 Condition of Test
Measurement Conditions
According to JIS Z 2241 Annex JB, the test is performed
at a strain rate of either 0.00007 s
-1
or 0.00025 s
-1
until the
upper yield point appears or measurement of proof
strength is completed. In case the upper yield point
appears, it is necessary to perform the test at a predicted
strain rate of either 0.00025 s
-1
or 0.002 s
-1
until the end of
discontinuous yielding. After measurement of the
required yield strength or proof strength, one of the
predicted strain rates of 0.00025 s
-1
, 0.002 s
-1
, or 0.0067 s
-1
is selected. In this test, the strain rate was set at 0.00007 s
-1
until completion of proof strength measurement, and
the predicted strain rate after the completion of proof
strength measurement was set at 0.002 s
-1
. Table 2 shows
the detailed test conditions.
According to JIS Z 2241 Annex JB, the strain rate must be
controlled within ±20 %. Unlike the conventional
software, the software TRAPEZIUM X-V has a function for
graphing the test speed during the test. This feature
enabled easy confirmation that the test speed during the
test satisfied the test standard.
Table 2 Test Conditions
Test speed : 0.00007 s
-1
0.002 s
-1
(changed at 1 % strain)
Gauge length : 50 mm
Number of tests : n = 3
Specimen shape : JIS Z 2241 No. 5 (thickness: 1 mm)
Specimen material : SPFC980
Measurement Results
Fig. 2 shows the actual strain rate. The part shown in gray
is the ±20 % permissible error region. The strain rate error
was ±10 % or less, indicating that testing can be
performed with extremely high accuracy.
Fig. 2 Example of Strain Rate in Test
Displacement 1 (strain) (%)
Strain rate (%/s)