User Benefits
Application
News
Compression Tests for Anode Material for
Lithium-Ion Batteries
The deformation strength can be calculated by performing compression tests on anode material one particle at a time.
This provides a useful method for correctly analyzing the physical properties of particulate material, without being affected by the
experience of the analyst.
This provides an index for evaluation of strength, for development of new anode materials.
Chika Oya
MCT™-510 Micro Compression Testing Machine
Introduction
Lithium-ion batteries are a type of rechargeable battery that is
charged or discharged by desorption or insertion of lithium ions
(Li
+
) from or into the active material structure. In recent years, the
uses of lithium-ion batteries have expanded dramatically, and
research to increase their capacity, extend their life, reduce their
cost, and increase their safety is being actively undertaken. The
main materials of lithium-ion batteries are the cathode, anode,
separator, and electrolytic solution, with the active material, the
main material from which the electrodes are composed, being the
most important element for improving performance.
In recent years the use of silicon and metal oxides as anode
materials has been investigated. Silicon anodes have a higher
theoretical capacity than conventional carbon anode materials, so
they are expected to contribute to higher capacity lithium-ion
batteries. On the other hand, charging and discharging can easily be
accompanied by volumetric expansion and contraction, so there is
the issue that aging of the battery itself is faster compared with
carbon anode materials.
Hence evaluation of the properties of new materials is required in
order to improve the performance of anode materials. In this article
a case of measurement of deformation strength
*1
in compression
tests is introduced, as an example of quantitative evaluation of
physical properties. The MCT-510 micro compression testing
machine is used for compression tests on minute samples and can
be applied to flexible anode materials. The deformation strength is
quantitatively evaluated by high-accuracy measurement of both
displacement and force.
Test Specimens
Table 1 shows information regarding the test specimens used in this
test, and Fig. 1 shows an image of a test specimen. When anode
material is dispersed on the test specimen stand with a spoon, each
particle can be observed using the instrument’s microscope, as
shown in Fig. 1(b).
Fig. 2 Test Apparatus and Schematic View of a Test
*1 Deformation strength
The strength as defined by JIS Z 8844 (Test method of fracture and deformation
strength of a fine particle), and is obtained by calculation from Equation (1).
Specimen : Three types of anode material (anode material a, anode
material b, anode material c)
Material : Carbon (graphite)
Particle diameter : 10-15 μm
Table 1 Test Specimen Information
Fig. 1 Test Specimen
(a) On the lower compression plate
(b) Particle observed with a 400 fold microscope
(a) (b)
Supplied by: Dainen Material Co., Ltd.
Indicates ∅50 μm
Specimen
Test Conditions
Fig. 2 shows a view of the instrument and a schematic diagram of a
test, and Table 2 shows the test conditions. With the MCT-510 it is
possible to perform a compression test on single particles, and use
the Side Observation Kit to view the compression on video.
The anode material used in this case was graphite, so it was soft,
and with this sample it was difficult to correctly determine the start
of the compression test when the particle was contacted. To resolve
this problem, the soft material measurement mode
*2
was used. The
following equation shows the calculation of deformation strength.
σ
10%
: Deformation strength for a 10 % compression displacement of
particle size [Pa]
F
10%
: Force for a 10 % compression displacement of particle size [N]
A : Representative area [m
2
]
(Area equivalent to a circle, found from the particle size measured
before compression)
d : Particle size [m]
=
π
2
4
σ
10%
=
10%
• • • (1)
Indenter
Force
Anode
material
Schematic View of Testing