Application
News
www.shimadzu.com/an/
Shimadzu Corporation
Analytical & Measuring Instruments Division
Global Application Development Center
© Shimadzu Corporation, 2022
For Research Use Only. Not for use in diagnostic procedures.
This publication may contain references to products that are not available in your country. Please contact us to check the availability of these
products in your country.
The content of this publication shall not be reproduced, altered or sold for any commercial purpose without the written approval of Shimadzu.
See http://www.shimadzu.com/about/trademarks/index.html for details.
Third party trademarks and trade names may be used in this publication to refer to either the entities or their products/services, whether or not they
are used with trademark symbol “TM” or “”.
The information contained herein is provided to you "as is" without warranty of any kind including without limitation warranties as to its accuracy or
completeness. Shimadzu does not assume any responsibility or liability for any damage, whether direct or indirect, relating to the use of this
publication. This publication is based upon the information available to Shimadzu on or before the date of publication, and subject to change
without notice.
First Edition: Mar. 2022 01-00023-EN
Fig. 6 Ratios of Constituent Sugars of CNF Samples
Table 6 Recovery Rates and Excessive Decomposition Correction Factors
for Monosaccharides
*7 In this analysis, the samples were hydrolyzed in sample preparation, and a
quantitative analysis of the monosaccharides was performed. Scale factor
is the coefficient that takes into account dehydration condensation.
Ratio of Constituent Sugars
Spike-and-recovery test, correction for excessive decomposition,
and calculation of polysaccharide were carried out using the
quantitative values of the detected saccharides. Fig. 6 shows the
composition ratio of each saccharide when the integrated value is
defined as 100.
Summary
It was possible to determine the ratios of the constituent sugars
in various CNF samples by analyzing the saccharides in the
samples after hydrolysis treatment using the Nexera reducing
sugar analysis system.
Differences in the types and amounts of constituent sugars could
be seen in the CNFs derived from different materials. As shown in
Fig. 7, cellulose is a polysaccharide which is polymerized by
glycosidic linkage of glucose, whereas the main components of
hemicellulose are the insoluble dietary fibers xylan, which is
formed by polymerization of xylose or other saccharides, and
mannan, which is formed by polymerization of glucose and
mannose. It is known that hemicellulose is distributed in large
amounts in broadleaf trees.
Analysis of Binfi-s (Sugino Machine Limited, Toyama, Japan)
produced from wood pulp showed that, a large amount of xylose
tends to be detected in addition to glucose. However, BCNFs such
as fermented nanocellulose, which are formed by bacteria from
the glucose in molasses or agricultural raw materials, consisted of
90 % or more glucose, and did not contain xylose, which has been
confirmed to originate from wood pulp.
Spike-and-Recovery Test, Correction for
Excessive Decomposition, and Calculation
of Polysaccharide
Because the saccharides in the samples may decompose due to
excessive decomposition during hydrolysis, it is necessary to
correct by performing a spike-and-recovery tests of the
monosaccharides. For this test, 8.4 mL of a mixed standard solution
of the monosaccharides (each saccharide: 500 μmol/L) was taken in
a 25 mL test tube, and 300 μL of 72 % sulfuric acid was added with a
pipette. Two test solutions were prepared. One (solution a) was
decomposed by heating in an autoclave for 1 hour at 120 ˚C
simultaneously with hydrolysis. After cooling, water was added to
the autoclaved solution until the total volume reaches 10 mL. The
other (solution b) was simply adjusted to 10 mL with water
without being heated in the autoclave. Both solutions were
diluted 4 times, after which quantitative analyses of solutions a
and b were performed, and the recovery rate of each
monosaccharide before/after hydrolysis was obtained. Correction
for excessive decomposition was carried out by multiplying the
monosaccharide concentration of the sample before correction
by the reciprocal of the recovery rate. Table 6 shows the recovery
rates and the excessive decomposition correction factors for each
monosaccharide. The calculation of polysaccharide was carried
out by multiplying the corrected monosaccharide concentration
by the scale factor of monosaccharide that is 0.9 for a hexose and
0.88 for a pentose.
*7
Compound Recovery rate (%)
Correction factor for the
excessive
decomposition
Xylose 87 1.15
Arabinose 92 1.08
Mannose 94 1.07
Glucose 95 1.06
Galactose 92 1.08
0%
20%
40%
60%
80%
100%
No.1 No.2 No.3 No.4 No.5 No.6 No.7 No.8
Xylose Arabinose Mannose Glucose Galactose Cellobiose
Glucose
Xylose
Mannose
Arabinose
Cell wall of plants
Cellulose
Hemicellulose
Hydrolysis
Hydrolysis
Fig. 7 Cellulose and Hemicellulose
<Acknowledgments>
We wish to express our profound thanks to the following persons for useful
discussion and various advice in connection with the development of this
analysis method and provision of the samples.
• The University of Tokyo: Special Research Professor Akira Isogai, Associate
Professor Tsuguyuki Saito, and Assistant Professor Shuji Fujisawa
• Hokkaido University: Associate Professor Kenji Tajima
• Kusano Sakko Inc.: Mr. Tokuo Matsushima, General Manager of
Nanocellulose/Agricultural Business
• Ehime University: Professor Hiromi Uchimura, Professor Tomoki Yabutani,
and Assistant Professor Akihiro Hideno
Nexera, Shim-pack and SHIMADZU LabTotal are trademarks of Shimadzu Corporation or its affiliated companies in Japan and/or other countries.