Content overflows the browser. Try zooming out (Ctrl + −) to see the full page. PDF Download
User Benefits Application News Fig. 2 Appearance of Samples Fig. 1 IRSpirit™-X with QATR™-S Installed Table 2 Analysis Conditions Fig. 4 Spectrum from the Transparent Bead Introduction In recent years, there has been increasing interest in plastic recycling internationally. The United States announced its National Recycling Strategy 1) on November 15, 2021, aiming to increase the recycling rate to 50% by 2030. In Europe, an amendment to Directive 94/62/EC on packaging and packaging waste 2) was announced on November 30, 2022, which proposes packaging waste reduction targets by 2040, the introduction of a common material labeling system, and a minimum recycled plastic content in plastic packaging. In Japan, the Plastic Resource Circulation Promotion Law came into effect on April 1, 2022. Various sorting technologies, such as density separation, electrostatic separation, near-infrared/infrared sorting, Raman spectroscopy sorting, and X-ray transmission density sorting are utilized in the process of plastic recycling. In particular, FTIR spectrophotometer used for infrared sorting, allows for accurate qualitative analysis of polymers and can identify polymers regardless of their color or form (powder/solid), making it useful for sorting a variety of plastics. Moreover, FTIR can be used not only for qualitative analysis during collection but also for confirming the ratios of different plastic types during the acceptance of recycled plastics and for detecting contaminants after molding. FTIR spectrophotometers are useful for qualitative analysis of a wide variety of plastics. With FTIR, it is possible to measure and analyze black or dark-colored plastics that cannot be measured by plastic automatic sorting devices that utilize near-infrared light. The Spectrum Advisor function ensures the acquisition of high-quality data. FTIR Analysis of Recycled Plastics Using the Spectrum Advisor Function Xu Yan and Karen Maruyama Fourier Transform Infrared Spectrophotometer IRSpirit™-X Samples and Analysis Conditions The transparent bead and black fragment used as plastic samples for this measurement are shown in Fig. 2. The analysis conditions are indicated in Table 1. The QATR-S was used as the ATR attachment. Transparent bead Black fragment Instruments : IRSpirit-TX and QATR ™ -S (Diamond, Ge) Resolution : 4 cm -1 Accumulation : 45 times Apodization Function : SqrTriangle Detector : DLATGS Qualitative Analysis of Transparent Bead The transparent bead was placed on the prism (Fig. 3) and spectra were obtained using the ATR method. The measurement result is shown in Fig. 4. The peaks derived from the bead were very weak, making qualitative analysis difficult. Therefore, the Spectrum Advisor function was used to investigate the cause. Fig. 3 Transparent Bead Pressed against the ATR Prism Spectrum Advisor IRSpirit-X series Fourier transform infrared spectrophotometers are compact and portable FTIR systems. Equipped with QATR™- S, a built-in single reflection ATR measurement unit, IRSpirit-X allows for easy measurement of variously shaped samples by simply pressing them onto the prism. However, since plastics brought for recycling come in various shapes, insufficient sample pressing may result in poor spectra and make qualitative analysis difficult. Additionally, spectra may also be affected by the atmospheric environment in some cases. The Spectrum Advisor function newly introduced in the IRSpirit-X series compares the measured spectra with case models and provides advice on parameters, accessories, and troubleshooting related to data processing. As a result, high- quality spectra can be acquired. In addition to describing examples of plastic measurements, this article also provides an overview of the Spectrum Advisor function.
Application News www.shimadzu.com/an/ Shimadzu Corporation © Shimadzu Corporation, 2023 For Research Use Only. Not for use in diagnostic procedures. This publication may contain references to products that are not available in your country. Please contact us to check the availability of these products in your country. The content of this publication shall not be reproduced, altered or sold for any commercial purpose without the written approval of Shimadzu. See http://www.shimadzu.com/about/trademarks/index.html for details. Third party trademarks and trade names may be used in this publication to refer to either the entities or their products/services, whether or not they are used with trademark symbol “TM” or “”. Shimadzu disclaims any proprietary interest in trademarks and trade names other than its own. The information contained herein is provided to you "as is" without warranty of any kind including without limitation warranties as to its accuracy or completeness. Shimadzu does not assume any responsibility or liability for any damage, whether direct or indirect, relating to the use of this publication. This publication is based upon the information available to Shimadzu on or before the date of publication, and subject to change without notice. First Edition: Dec. 2023 01-00653-EN IRSpirit and QATR are trademarks of Shimadzu Corporation or its affiliated companies in Japan and/or other countries. References 1) National Recycling Strategy (Referenced Oct. 2023) https://www.epa.gov/system/files/documents/2021-11/final- national-recycling-strategy.pdf 2) Regulation of the European Parliament and of the Council (Referenced Oct. 2023) https://eur-lex.europa.eu/legal- content/EN/TXT/HTML/?uri=CELEX:52022PC0677 Fig. 10 Spectra from the Black Fragment and Search Result Fig. 5 Investigation by the Spectrum Advisor Function (Transparent Bead) Qualitative Analysis of the Black Fragment The measurement result from the black fragment is shown in Fig. 8. Peaks originating from the sample were obtained, but distortion was observed around 800 cm -1 , and the baseline was rising toward the right side. Therefore, the transparent bead was remeasured with the flat side held in close contact with the prism (Fig. 6). The result is shown in Fig. 7. Center of the bead (dented) Fig. 6 Change in How the Transparent Bead was Positioned on the Prism — Transparent bead — Search result (polypropylene) Fig. 7 Spectra from the Transparent Bead and Search Result By simply changing the sample placement, a good spectrum was obtained and the search result indicated that the transparent bead was probably polypropylene. ー 黒色片 Peak distortion Rising baseline Fig. 8 Spectrum from the Black Fragment Samples that contain carbon black have a higher refractive index, which can result in peak distortions and rising baselines in spectra. In such cases, a germanium (Ge) prism, with a higher refractive index, is suggested to be used instead of a diamond prism. Fig.10 shows the spectrum obtained with a Ge prism. — Black fragment — Search result (SBR+CaCO 3 ) By changing the prism to Ge, a better spectrum was obtained, with the search result suggesting that the sample was probably a styrene-butadiene rubber (SBR) with an addition of calcium carbonate (CaCO 3 ). Conclusion In this study, recycled plastics were analyzed using the ATR method. By utilizing the Spectrum Advisor function, which is included as a standard feature, even individuals with limited measurement experience can perform accurate qualitative analysis regardless of the type or shape of the sample. Furthermore, FTIR allows for the qualitative analysis of various plastics, including black or dark-colored plastics, which would be difficult to analyze using automatic plastic sorting devices based on near-infrared light. This demonstrates its utility for sorting recycled plastics. “Samples-derived peaks not detected“ was selected on the following Spectrum Advisor screen, resulting in the suggestion that “the sample and ATR prism may have poor adherence” (Fig. 5). In this case, it was determined that the transparent bead has a dent in the center, that resulted in poor adherence and a poor spectrum. Fig. 9 Investigation by the Spectrum Advisor Function (Black Fragment) In this case, “Baseline position is a larger value the lower that the wavenumber side becomes (absorbance display)” was selected in Spectrum Advisor, resulting in the suggestion “A large amount of carbon black may be included” (Fig. 9). Side of the bead
Please fill out the survey Related Products Some products may be updated to newer models. IRSpirit-X Series Related Solutions Chemicals (Archive)Plastics Price Inquiry Product Inquiry Technical Service / Support Inquiry Other Inquiry Powered by TCPDF (www.tcpdf.org)