Application
News
www.shimadzu.com/an/
Shimadzu Corporation
© Shimadzu Corporation, 2025
For Research Use Only. Not for use in diagnostic procedures.
This publication may contain references to products that are not available in your country. Please contact us to check the availability of these
products in your country.
The content of this publication shall not be reproduced, altered or sold for any commercial purpose without the written approval of Shimadzu.
See http://www.shimadzu.com/about/trademarks/index.html for details.
Third party trademarks and trade names may be used in this publication to refer to either the entities or their products/services, whether or not
they are used with trademark symbol “TM” or “”.
Shimadzu disclaims any proprietary interest in trademarks and trade names other than its own.
The information contained herein is provided to you "as is" without warranty of any kind including without limitation warranties as to its
accuracy or completeness. Shimadzu does not assume any responsibility or liability for any damage, whether direct or indirect, relating to the
use of this publication. This publication is based upon the information available to Shimadzu on or before the date of publication, and subject
to change without notice.
LabSolutions is a trademark of Shimadzu Corporation and its affiliates in Japan and/or other countries.
UV irradiation time
10 h
15 h
20 h
25 h
30 h
0 h
1 h
2 h
3 h
5 h
UV irradiation time
0 h
10 h
15 h
30 h
Hazen Scale-Based Evaluation of UV-Degraded
Plastics
LabSolutions UV-Vis Color, an optional software product for
LabSolutions UV-Vis, can calculate Hazen unit values.
Information on configuring advanced settings in the software to
calculate Hazen unit values can be found in Application News
No. 01-00834-EN.
The total transmittance spectra of the PC and PET samples were
used to calculate Hazen unit values and the samples were
evaluated based on these values. The Hazen unit values
calculated from the spectra are shown in Tables 2 and 3.
Similar to PC, Fig. 5 shows the longer PET is irradiated with UV
light the greater the loss of transmittance.
Fig. 6 shows an overlay of the total transmittance spectra of the
PC and PET samples after 0, 10, 15, and 30 hours of UV
irradiation. Comparing unirradiated (0 h) PC (solid red line) and
unirradiated (0 h) PET (dashed red line) reveals that at
wavelengths below 450 nm, PC transmittance was higher than
PET transmittance, indicating that PC is a more transparent
material. Also, while unirradiated PC and PET transmittance was
almost identical at wavelengths above 450 nm, PET
transmittance was lower than PC transmittance after an
equivalent length of UV irradiation, and the irradiation had a
greater yellowing effect on PET than PC.
Fig. 5 Total Transmittance Spectra of UV-Degraded PET
Table 2 Hazen Unit Values Calculated for UV-Degraded PC
Fig. 6 Comparing Total Transmittance Spectra of UV-Degraded PC and PET
Solid Lines: PC, Dashed Lines: PET
0
50
100
150
200
250
300
350
0 10 20 30
Hazen unit value
UV irradiation time (h)
PC
PET
<Related Application News Articles>
1. Using UV-1900i Plus to Evaluate Raw Materials for Chemical
Products Based on the Hazen Color Scale
Application News No. 01-00834-EN
2. Analysis of Ultraviolet-Degraded Plastic by Plastic Analyzer
Application News No. A647
Conclusion
Hazen unit values were calculated for the yellowing caused by
UV irradiation of two highly transparent plastics (PC and PET).
The relationship between these Hazen unit values and the
duration of UV irradiation showed that PET was degraded by UV
light more quickly than PC.
LabSolutions UV-Vis Color includes a calibration curve for
calculating Hazen unit values, allowing the user to calculate
Hazen unit values simply by measuring sample transmittance
and without needing to measure the transmittance of
numerous standard samples.
Finally, while standards such as ISO 6271:2015
1)
, ASTM D1209-
05(2019)
2)
, and JIS K0071-1:2017
3)
include criteria related to the
Hazen scale, when evaluating a material based on any of these
or similar standards, verifying that these standards are the latest
versions of those standards is recommended.
Fig. 9 shows the relationship between the Hazen unit values in
Tables 2 and 3 and the UV irradiation time.
Fig. 9 Hazen Scale-Based Evaluation of UV-Degraded PC and PET
The Hazen unit values for PET increased faster with UV irradiation
time than for PC, indicating that PET is more susceptible to UV
degradation. Also, while the increase in Hazen unit values with UV
irradiation time was almost entirely linear for PC, for PET the
increase in Hazen unit values slowed from 20 hours onward.
Table 3 Hazen Unit Values Calculated for UV-Degraded PET
First Edition: Feb. 2025 01-00835-EN
<References>
1. ISO 6271:2015 Clear liquids — Estimation of colour by the
platinum-cobalt colour scale
2. JIS K0071-1:2017 Test methods for colour of chemical
products—Part 1: Estimation of colour in Hazen units
(platinum-cobalt colour scale)
3. ASTM D1209-05(2019) Standard Test Method for Color of Clear
Liquids (Platinum-Cobalt Scale)