Content overflows the browser. Try zooming out (Ctrl + −) to see the full page. PDF Download
Application Note No. 14 UV Degradation Analysis of Material for Solar Cell Modules Using GC/MS and FTIR Y. Katayama, S. Takeuchi Electrics and Electronics LAAN-C-XX-E028 1. Introduction Materials for solar cell modules are expected to maintain their performance for over a decade despite the harsh environmental conditions such as high temperatures and ultraviolet irradiation to which they are subjected outdoors. However, there is concern that UV-induced degradation may occur in materials used in modules such as ethylene-vinyl acetate (EVA) which is a copolymer used as a clear encapsulation film. This article introduces three example analyses: analysis of EVA film subjected to intense UV irradiation using a UV (ultraviolet) -Py (double-shot pyrolyzer) / GC-MS (gas chromatograph mass spectrometer) system, evolved gas analysis by mass spectrometry (EGA-MS) of EVA film which was degraded by UV irradiation in the same way as with the above, and analysis of the same using a Fourier transform infrared spectrophotometer (FTIR). Fig. 1 Structural formula of ethylene-vinyl acetate (EVA) copolymer Analytical Applications Department, Analytical & Measuring Instruments Division EVA: ethylene-vinyl acetate copolymer CH 2 CH 2 n CH 2 CH m O C CH 3 O
2 Application Note No. 14 2. UV degradation of EVA film using a UV-Py/GC-MS system The UV-Py/GC-MS system shown in Fig. 2 was made by combining a micro-UV irradiator (UV-1047 Xe) manufactured by Frontier Laboratories Ltd., and the GCMS-QP2020 gas chromatograph mass spectrometer manufactured by Shimadzu Corporation. Compared to conventional weather testing methods such as outdoor exposure testing and weatherometer testing, this system enables rapid UV degradation of EVA film. In addition, this UV-Py/GC-MS system is capable of performing GC/MS analysis of volatile degradation products which are generated due to UV irradiation. Degradation samples can be analyzed employing evolved gas analysis by mass spectrometry (EGA-MS), a method available with the Py/GC-MS, and by using a Fourier transform infrared spectrophotometer (FTIR) to elucidate the changes in the resin structure that are induced by UV irradiation. Fig. 3 shows the procedure for UV degradation of EVA film using the UV-Py/GC-MS system. Fig. 2 UV-Py/GC-MS system (UV-1047Xe+PY-3030D+GCMS-QP2020) Fig. 3 Measurement flow for UV-Py/GC-MS analysis FTIR analysis EGA-MS analysis (1) Analysis of changes in material properties before and after UV irradiation through evolved gas analysis by mass spectrometry (EGA-MS) Molecular structure analysis of EVA in the vicinity of the film surface by total reflectance spectroscopy (ATR method) Py/GC-MS system (PY-3030D+GCMS-QP2020) IRAffinity-1S Fourier transform infrared spectrophotometer Weigh out approx. 2 mg of the sample and place the sample in the dedicated Eco-cup. (1) Weighing Set the dedicated Eco-cup in the UV sampler. Fill the furnace with air. (2) Setting the cup in the instrument (3) UV irradiation Immerse the column in liquid nitrogen and perform UV irradiation. This research was done using irradiation times of 0, 1, 2, and 5 hours. In order to purge the air inside the column with helium, wait for 15 minutes after switching to helium. (4) Purging with helium After connecting the column to the mass spectrometer, take the column out from the liquid nitrogen and perform analysis. (5) GC/MS analysis After analysis, take the degradation sample out from the UV sampler. (6) Collection of degradation sample (2) (3) (4) (5)
UV Degradation Analysis of Material for Solar Cell Modules Using GC/MS and FTIR 3 3. Analysis of volatile degradation products using the UV-Py/GC-MS system 3-1 Overview Volatile degradation products generated through UV irradiation were analyzed using the UV-Py/GC-MS system. Whereas evaluation of gas generated during degradation is not possible if employing methods such as outdoor exposure testing or weatherometer testing, evaluation of such gas is possible if using a UV-Py/GC-MS system. Fig. 4 shows the schematic of the UV-Py/GC-MS system. Analysis is done with this system by first setting the sample inside the furnace that is filled with air and then cooling the inlet of the column using liquid nitrogen. After performing UV irradiation for the set time, the evolved gas generated during the light-induced degradation of the sample is collected. Subsequently, the air in the instrument is purged with helium and the column is connected to the mass spectrometer. After taking the column out from the liquid nitrogen, the evolved gas collected in the cooled section of the column is analyzed. Fig. 4 Schematic of the UV-Py/GC-MS system 3-2 Analysis conditions Table 1 lists the analysis conditions for volatile degradation products using the UV-Py/GC-MS system. Table 1 Analysis conditions for volatile degradation products using the UV-Py/GC-MS system Instrument <Conditions for the UV-Py> Irradiation time 0 hr, 1 hr, 2 hr, 5 hr Helium purging time 15 min Pyrolyzer furnace temperature 60 °C Atmospheric gas Air <Conditions for the GC> Column Ultra ALLOY-1 (30 m L. × 0.25 mm I.D. df=0.5 μm) manufactured by Frontier Laboratories Injection port temperature 300 °C Column temperature 40.0 °C → 20.0 °C /min → 300.0 °C (5.00 min) Injection mode Split mode Carrier gas Helium Carrier gas pressure 50 kPa Split ratio 40:1 <Conditions for the MS> Ion source temperature 200 °C Interface temperature 300 °C Measurement mode SCAN Measurement range m/z 29-1090 Event time 0.5 sec Approx. 2 mg of sample Helium Air UV-Py unit GC injection port Separation column Liquid nitrogen Sample Volatile degradation products UV light Air for UV irradiation Helium for analysis MS unit GC unit Furnace temperature 60 °C UV irradiation
4 Application Note No. 14 3-3 Analysis results The result of analyzing the volatile degradation products generated through UV irradiation (0, 1, 2, 5 hours) using the UV-Py/GC-MS system is shown in Figs. 5 to 8. Underlined compounds in the figures are compounds which are considered to be volatile degradation products of EVA. Fig. 5 UV-Py/GC-MS analysis results of volatile degradation compounds generated through UV irradiation (0 hours) Fig. 6 UV-Py/GC-MS analysis results of volatile degradation compounds generated through UV irradiation (1 hour) Fig. 7 UV-Py/GC-MS analysis results of volatile degradation compounds generated through UV irradiation (2 hours) Fig. 8 UV-Py/GC-MS analysis results of volatile degradation compounds generated through UV irradiation (5 hours) CO 2 Hexamethylcyclotrisiloxane (D3) Octamethyltetrasiloxane (D4) Tetradecamethylcycloheptasiloxane (D7) Hexadecamethylcyclooctasiloxane (D8) Irradiation time: 0 hours 2.5 5.0 7.5 10.0 12.5 15.0 17.5 min Acetone CO 2 Formaldehyde+Propylene Acetaldehyde Butene Aceton Isopropyl alcohol Butanol Acetic acid Unknown Ethanol 2.5 5.0 7.5 10.0 12.5 15.0 17.5 min Irradiation time: 1 hour CO 2 +Formaldehyde+Propylene Acetaldehyde Butene Aceton Isopropyl alcohol Butanol Acetic acid Ethanol Heptadiene Diacetylethane Undecadiene Dodecadiene Unknown Octadiene 2.5 5.0 7.5 10.0 12.5 15.0 17.5 min Irradiation time: 2 hours CO 2 Formaldehyde+Propylene Acetone Acetaldehyde Butene Isopropyl alcohol Butanol Acetic acid Ethanol Heptadiene Diacetylethane Undecadiene Dodecadiene Octadiene Octamethyltetrasiloxane (D4) +Decene Unknown 2.5 5.0 7.5 10.0 12.5 15.0 17.5 min Irradiation time: 5 hours
UV Degradation Analysis of Material for Solar Cell Modules Using GC/MS and FTIR 5 3-4 Expected light decomposition reaction of EVA Based on Figs. 5 to 8, we can assume that compounds that have a greater peak area under a longer UV irradiation time are a product of light decomposition. Since the EVA film used for analysis hardly contained any additives, we were able to observe the light decomposition of the EVA film itself and therefore infer the light decomposition reaction as shown in Fig. 9. Fig. 9 The light decomposition reaction of EVA inferred based on measurement results CH 2 CH 2 n CH 2 CH m O C CH 3 O Ethylene-vinyl acetate copolymer CH 2 CH 2 n CH m CH + CH 3 C OH Propylene Butene Heptadiene Octadiene Nonadiene Decadiene Undecadiene Dodecadiene . . . . Acetic acid CH 2 CH 2 n CH 2 C m O CH 3 C H O CH 2 C OH O CH 3 C CH 3 O H C H O CH 3 C CH 2 CH 2 O C CH 3 O , , , Acetaldehyde Acetone Formaldehyde Diacetylethane CH 2 CH 2 n CH 2 CH m . O CH 3 C . O + + CH 2 CH OH Ethanol Isopropyl alcohol Butanol . . . . O Light decomposition
6 Application Note No. 14 4. Analysis of UV-irradiated EVA through evolved gas analysis by mass spectrometry (EGA-MS) 4-1 Overview Changes in the properties of EVA film from before and after UV irradiation were analyzed through evolved gas analysis by mass spectrometry (EGA-MS), which is a method that is available with a Py/GC-MS configuration. Fig. 10 shows the schematic of the EGA-MS system. Analysis by the EGA-MS method is done by connecting the outlet of the pyrolyzer with the GC detector using the inactivated tube (Ultra ALLOY, 2.5 m L. × 0.15 mm I.D.) installed inside the GC oven and then detecting, in real time, the various substances that are generated from the sample through heating. By comparing the thermal decomposition temperatures of the degraded EVA film, it is possible to reveal the degree of cleavage reactions on the main chain that are caused by UV irradiation. 4-2 Analysis conditions The conditions for analyzing UV-irradiated EVA by EGA-MS are listed in Table 2. Fig. 10 Schematic of the EGA-MS system Table 2 Analysis conditions for EGA-MS Instrument <Conditions for the Py> Pyrolyzer furnace temperature 40.0 °C (2.00 min) → 20 °C /min → 750.0 °C (2.50 min) Interface temperature Auto (Upper Temp. 320 °C) <Conditions for the GC> Column Ultra ALLOY-DTM (2.5 m L. × 0.15 mm I.D., no liquid phase) manufactured by Frontier Laboratories Injection port temperature 320 °C Column temperature Constant at 300 °C Injection mode Split mode Carrier gas Helium Carrier gas pressure 120 kPa Split ratio 40:1 <Conditions for the MS> Ion source temperature 250 °C Interface temperature 320 °C Measurement mode SCAN Measurement range m/z 29-1090 Event time 0.5 sec Py unit EGA tube GC oven (constant at 300 ˚C) GC injection port Carrier gas MS unit GC unit Approx. 0.5 mg of sample Furnace temperature 40 to 750 ˚C
UV Degradation Analysis of Material for Solar Cell Modules Using GC/MS and FTIR 7 4-3 Analysis results The EGA-MS analysis results of EVA film degraded by UV irradiation per each irradiation time are shown in Fig. 11. The thermal decomposition temperature for each of the UV irradiation times is listed in Table 3. We can see that a longer UV irradiation time results in a slightly lower thermal decomposition temperature for peak (2), meaning that the molecular weight is decreasing. This indicates that light decomposition is occurring on the main chain of the EVA film due to UV irradiation. In addition, the difference in the absolute intensity of the thermal decomposition of the main chain (peak (2)) between each UV irradiation time was subtle. From this, we can assume that light decomposition is occurring only on the surface of the EVA film and not the entirety of the film. Fig. 11 EGA-MS analysis results of EVA film degraded under different UV irradiation times Table 3 Thermal decomposition temperature of main chain under different UV irradiation times UV irradiation time 0 hr 1 hr 2 hr 5 hr Thermal decomposition temperature (°C) 465.5 463.7 463.9 461.9 5. Analysis of UV-irradiated EVA using a Fourier transform infrared spectrophotometer (FTIR) 5-1 Overview Structural changes that occur in compounds through degradation can be analyzed using a Fourier transform infrared spectrophotometer (FTIR). Although the samples used in this research were only about 2 mm square in size, the surface spectrum of these samples can be measured easily by using the single reflection ATR accessory. This section introduces the results obtained by installing the DuraSamplIR II, which is a single reflection ATR accessory, on Shimadzu's IRAffinity-1S Fourier transform infrared spectrophotometer and measuring samples which were UV-irradiated for 0, 2, and 5 hours respectively. Fig. 12 IRAffinity-1S Fig. 13 DuraSamplIR II ˚C 40 100 200 300 400 500 600 700 0 hr 1 hr 2 hr 5 hr (1) Detachment of side chain (2) Thermal decomposition of main chain
First Edition: Jan. 2018 For Research Use Only. Not for use in diagnostic procedures. This publication may contain references to products that are not available in your country. Please contact us to check the availability of these products in your country. The content of this publication shall not be reproduced, altered or sold for any commercial purpose without the written approval of Shimadzu. Shimadzu disclaims any proprietary interest in trademarks and trade names used in this publication other than its own. See http://www.shimadzu.com/about/trademarks/index.html for details. The information contained herein is provided to you "as is" without warranty of any kind including without limitation warranties as to its accuracy or completeness. Shimadzu does not assume any responsibility or liability for any damage, whether direct or indirect, relating to the use of this publication. This publication is based upon the information available to Shimadzu on or before the date of publication, and subject to change without notice. © Shimadzu Corporation, 2018 www.shimadzu.com/an/ 5-2 Analysis results The spectra obtained by measuring the samples which were UV-irradiated for 0, 2, and 5 hours respectively are superimposed in Fig. 14. Changes with regard to functional groups can be observed: a decrease of the >C=O group originating from acetate in the vicinity of 1735 cm -1 , an increase of the >C=O group originating from ketone and aldehyde in the vicinity of 1716 cm -1 , and an increase in the peak intensity of the -OH group in the vicinity of 3300 cm -1 . Fig. 15 (a), (b), and (c) depict these peak changes by plotting them against the UV irradiation time. Each graph is based on the peak at 1465 cm -1 (CH2 and CH3 bending), with graphs (a) and (b) plotting the peak intensity ratio and graph (c) plotting the peak area ratio. For each sample, both the front and back sides are measured and plotted respectively. These results indicate that the side chain structure of EVA changed at the sample surface due to UV irradiation, thereby generating compounds containing the -OH group or the >C=O group originating from aldehyde or ketone. Fig. 14 IR absorbance spectra of EVA film before and after UV irradiation Fig. 15 Changes in functional groups (a) acetate, (b) ketone and aldehyde, and (c) O-H due to UV irradiation 6. Summary We clarified the volatile degradation products which result from EVA film due to UV irradiation by measuring EVA film using a UV-Py/GC-MS system. We also were able to estimate the decomposition behavior of the main and sub chains through evolved gas analysis by mass spectrometry (EGA-MS) according to changes in the UV irradiation time and evaluate changes in functional groups based on the results obtained through FTIR. Both of these methods are effective in investigating the decomposition behavior of resin structures induced by UV irradiation. * This publication is based upon the information available to Shimadzu on or before the date of publication, and subject to change without notice. C=O E V A _ 0 h r 2 E V A _ 2 h r 2 E V A _ 5 h r 2 0 . 4 0.3 0.2 0.1 0 A b s 4 0 0 0 3 5 0 0 3 0 0 0 2 5 0 0 2 0 0 0 1 7 5 0 1 5 0 0 1 2 5 0 1 0 0 0 7 5 0 E V A , 6 0 ˚C , U V : 5 h r 1 / c m O-H Absorbance ratio (A1735 / A1465) Absorbance ratio ( A1716 / A1465) Area ratio (3622-3120 / 1490-1402) 4 Abs 3.75 3.5 3.25 3 0 2.5 5 (a) 0 2.5 5 (b) 0 2.5 5 (c) 1 Abs 0.75 0.5 0.25 0 0.5 Corr. Area UV irradiation time (h) UV irradiation time (h) UV irradiation time (h)
Related Products Some products may be updated to newer models. IRAffinity-1S Fourier Transform Infrared Spectrophotometer Related Solutions Electronics Price Inquiry Product Inquiry Technical Service / Support Inquiry Other Inquiry Powered by TCPDF (www.tcpdf.org)