Application
News
www.shimadzu.com/an/
Shimadzu Corporation
© Shimadzu Corporation, 2026
For Research Use Only. Not for use in diagnostic procedures.
This publication may contain references to products that are not available in your country. Please contact us to check the availability of these
products in your country.
The content of this publication shall not be reproduced, altered or sold for any commercial purpose without the written approval of Shimadzu.
See https://www.shimadzu.com/about/trademarks/index.html for details.
Third party trademarks and trade names may be used in this publication to refer to either the entities or their products/services, whether or not
they are used with trademark symbol “TM” or “”.
Shimadzu disclaims any proprietary interest in trademarks and trade names other than its own.
The information contained herein is provided to you "as is" without warranty of any kind including without limitation warranties as to its
accuracy or completeness. Shimadzu does not assume any responsibility or liability for any damage, whether direct or indirect, relating to the
use of this publication. This publication is based upon the information available to Shimadzu on or before the date of publication, and subject to
change without notice.
First Edition: Oct. 2026 01-01280-EN
Conclusion
SSRM measurements enabled the visualization of local
resistance distributions in an n-type Si sample and a liquid LIB
positive electrode. Because SSRM provides current and
resistance distribution information over a wide range,
something not achievable with conventional current
measurements, the method is expected to be further used for
improving the performance of semiconductors and batteries.
References
1) N. Duhayon et al., “Assessing the performance of two-
dimensional dopant profiling techniques”, JVSTB 22, 385
(2004).
Acknowledgement
We are deeply grateful to Hiroshi Itoh of the National Institute of
Advanced Industrial Science and Technology (AIST) for providing
the n-type Si sample and for his guidance on the evaluation.
SSRM Measurement of Liquid LIB Positive
Electrode
Fig. 6 shows the SSRM measurement results of the liquid LIB
positive electrode. The display ranges are 10
-4
to 10
-10
A for
current and 10
5
to 10
11
Ω for resistance. In the topographic
image (a), the fine particle shapes of the active material and its
surroundings are observed. In the current image (b) and
resistance image (c), the current and resistance values differ
among active material particles. Focusing on active material
particles (1) to (3) outlined in white, the median resistance
values are (1) 4.57 × 10
8
Ω, (2) 3.89 × 10
9
Ω, and (3) 1.26 × 10
10
Ω.
The high-resistance particle (3) may be electrically isolated by
cracks inside the particle or by gaps between the particle and its
surroundings. Uneven resistance is also observed within the
same particle. Furthermore, in the resistance image, the black
regions of particularly low resistance are thought to be the
conductive additive, while the bright yellow regions of
particularly high resistance are thought to be the embedding
resin. In the current image (d), displayed over a range equivalent
to the conventional current-mode detection range, the current
saturates in both the conductive additive and the active
material, making it impossible to distinguish conductivity
differences. SSRM effectively detects small current changes
within large current variations, as shown by this sample.
Fig. 6 SSRM Measurement Results of Liquid LIB Positive Electrode
(a) Topographic image, (b) Current image, (c) Resistance image,
(d) Current image displayed in a range equivalent to the current detection range of the conventional current mode
(e) 3D overlay of topographic and current images, (f) 3D overlay of topographic and resistance images
(a) (b) (c)
(f)
(1)
(3)
(2)
(e)
XY: 30 µm
Z: 1 µm
(d)
XY: 30 µm
Z: 1 µm
Related Applications
1. Analysis of Positive Electrode (NCM) for Lithium Ion Battery by
EPMA and SPM, Application News No. P 117
(1)
(3)
(2)
(1)
(3)
(2)
SPM-9700HT is a trademark of Shimadzu Corporation and its affiliated companies in Japan and/or other countries.